QCM shows 100 nm and the witness measures 128 nm. How should tooling change?

A coating system receives a new lot of quartz monitor crystals of the same specification. Its controller closes the shutter at 100 nm, but an independent step-height instrument reads 128 nm. Purchasing asks whether the crystal is wrong. Process engineering considers lowering the density setting. Either change affects future lots. Trace the measurement through crystal frequency, film at the sensor and thickness at the product station. Establish where the difference originates before changing the crystal, material parameters or tooling factor.

Identify where each instrument measured

The quartz crystal microbalance (QCM) responds to mass deposited on it. The controller uses its frequency change and material parameters to estimate thickness. The monitor crystal is in a sensor head and the product is on a different holder. Even with the same shutter and deposition interval, source distance, angle, masking, substrate rotation and plume distribution can create different deposition rates. Kurt J. Lesker’s process equipment notes describe the tooling factor as a correction for this geometric difference. Moving the sensor or changing the chamber can invalidate the old factor.

Film density converts mass per area to thickness. The Z-ratio corrects acoustic impedance effects and can affect conversion as coating accumulates on the crystal. Both influence displayed thickness. To measure geometry, first fix the material, process and controller algorithm, then measure a reference sample. Changing density, Z-ratio and tooling in one trial can produce a correct display without identifying the correction that helped. The combination may not reproduce after a source, film material or monitor crystal change.

Convert the 100 nm and 128 nm readings into a parameter

Section 10.3 of the INFICON SQC-310 manual gives new tooling percent as initial tooling percent multiplied by actual substrate thickness divided by displayed thickness. Using 100 nm and 128 nm as an example, an initial 90% setting becomes 90% × 128/100 = 115.2%. Starting at 100% would give 128%. A film 28% thicker than displayed does not automatically call for adding 28 percentage points. For the actual controller version, check whether the field applies to the system, the film recipe or a sensor channel. Change the identified factor and export the before and after recipe.

Run a separate witness substrate with the new setting at the product station, through the prescribed stop condition, then measure it independently. A shutter triggered by displayed thickness now closes at a different time, so the previous run cannot qualify the corrected process by itself. Compare thickness at the setpoint, actual closing time, independent thickness after cooling and raw frequency. Before copying a percent setting from one controller to another, check field definitions, interactions with system settings and rounding. Reciprocal conventions can assign different numbers to the same physical correction.

When to check the shutter and thickness measurement

Use two thickness targets to see whether one multiplier explains the difference. At the old setting, suppose a 100 nm display gives 126 nm on the substrate and 200 nm gives 226 nm. The ratios are 1.26 and 1.13 while both differences are 26 nm. This illustrative pattern suggests fixed extra deposition or a thickness measurement zero offset. Check whether deposition continues after the shutter closes, whether the witness was exposed during source conditioning, whether the mask lifted the step edge and whether the independent instrument was calibrated. Then test a third thickness. If three different thicknesses give closely agreeing ratios with sufficient repeatability, a location-specific multiplier is more credible.

The product lot itself can be nonuniform across positions. Plot thickness using witness pieces at the critical holder locations. If the centre passes and the edge is thin, a common multiplier changes the displayed values without changing the physical thickness ratio. Review position, rotation or deposition uniformity, then choose a product reference location for tooling. If witness substrates and production substrates have different adsorption or growth behaviour, verify that the step-height or optical measurement represents the product. Link the units, measurement positions and sensor locations to the recorded results.

To diagnose the change of monitor crystals, retain fresh crystal frequencies from both lots, mounting photographs, sensor cleanliness, controller frequency limits, frequency traces and any sensor change alarms. Check the maker’s starting frequency, electrode and holder compatibility with the process. Compare witness runs on the same holder and recipe. If the error follows the crystal lot and does not match the geometry, send the manufacturer the complete record. If it appears after a holder change, check position and shutter geometry first.

Record uncertainty along with the 115.2% result. In the same example, suppose independent thickness measurement has standard uncertainty of 1.5 nm and display repeatability is equivalent to 2.0 nm. Treat the old setting as fixed. If the contributions are independent, relative standard uncertainty is approximately √[(1.5/128)² + (2.0/100)²], or 2.3%. This is about 2.7 percentage points on the new setting. One witness run may have insufficient margin to verify a ±3% product tolerance. Plan retests based on actual repeatability, thickness traceability and position variation. An extra decimal place in the recipe does not improve those quantities. Check for correlation if the reference and display measurements share a calibration process.

The qualification file should let someone reproduce which crystal and sensor head were used with which recipe and product station. Record the settings, measured values, material parameters, qualified thickness range and independent measurement uncertainty. A contract limit of nominal film thickness ±3% applies where the contract specifies it, such as the product station. Sign against the results there. Fine controller display resolution still needs a fresh witness to show whether the actual process meets the film-thickness tolerance.

WeChat